A workable starting point for web tension settings comes from two numbers, not one: the tension per unit width the film supplier recommends, and the width you are actually running. Everything else on the press — taper, infeed isolation, rewind build — exists to hold that figure steady from the first metre of the roll to the last. Get those two numbers wrong and no amount of operator attention will hold register for a full shift.
Most tension arguments on a production line are really arguments about units. One side quotes a brake force in newtons, the other a figure in newtons per metre, and the two never meet. Getting the units straight is the cheapest improvement available before any mechanical change is considered.
Key Takeaways
- Set tension per unit width, then convert to the force the machine needs at that web width.
- Film type sets the window through modulus: the same elongation needs far less force on polyethylene than on polyester.
- Adjust the infeed zone before the unwind, because infeed isolates the printing section from roll dynamics.
- A setting that needs constant manual correction is usually compensating for a roller, a gauge band or a splice rather than a wrong number.
What a tension setting actually controls
It controls elongation, and elongation controls everything downstream: register between stations, the position of the eye mark at the sealing jaws, and the flatness of the web as it enters the dryer. The machine displays force, but the process cares about strain.
That is why two presses can run the same film at the same displayed tension and produce different print lengths. Roller friction, web path length and the number of idlers all change how much of the brake force actually reaches the printing section.
Why the figure belongs per unit width
A force spread over a narrow web produces more strain than the same force spread over a wide one. Quoting tension per unit width removes the width from the equation, so the number can travel between jobs and between machines. When a job moves from a 1,000 mm web to a 600 mm web and the operator keeps the same brake pressure, the strain rises by roughly the ratio of the widths, and the register shows it.
The conversion is simple arithmetic once the supplier figure is in newtons per metre: multiply by the web width in metres to get the force to dial in. What is not simple is trusting the number afterwards, because the actual tension at the print nip is lower than the setpoint whenever the web passes over driven rollers or tight idlers.
How PET, BOPP and PE differ in their window
Polyester is stiff, so it tolerates a relatively high tension per unit width without much elongation, which makes it the easiest of the three to register. Biaxially oriented polypropylene sits in the middle and is dimensionally stable in the machine direction until it is heated, at which point it shrinks and the register moves. Polyethylene has the lowest modulus of the three, so the same tension per unit width produces much more stretch, and the window between “too slack to track” and “stretched enough to drift” is narrow.
Laminates add a second layer of behaviour. A PET and PE laminate follows the PET for stiffness at low tension and the PE once the tension is high enough to load the sealant layer. That transition is one reason a laminate can run cleanly at one speed and wander at another without any change to the setpoint.
Which zone to adjust first
Start with the infeed zone between the unwind and the first print unit. Its job is to deliver a consistent web to the printing section regardless of what the unwind is doing, so a stable infeed makes every later adjustment easier to read. If the infeed cannot hold its setpoint, no amount of tuning downstream will produce a stable register.
Then set the unwind to a value that keeps the infeed in its working range across the roll, and only then touch the rewind. Rewind is often adjusted first because it is the zone closest to the operator, and that order makes the diagnosis harder: a rewind problem then looks like a print problem.
Taper as the roll diameter falls
Brake torque and tension are not the same thing. As an unwind roll empties, the same torque produces a higher tension, so a fixed setpoint quietly over-tensions the last part of the roll. Taper reduces the setpoint as the diameter falls to keep the tension roughly constant, and it is the reason the end of a roll can behave differently from the beginning even on a well-set press.
Check the taper whenever a job shows drift that grows through the roll. If the drift resets when a new roll is loaded and then grows again, the taper or the diameter sensing is the first thing to examine, before the film is blamed.
How do you find a starting point on an unfamiliar film?
Use the supplier’s tension table as the anchor, then confirm it against the machine’s own limits. Run a short length at the lower end of the recommended range, check the print length at two stations and look at the web between idlers for slack or edge curl. Raise the tension in small steps until the web tracks flat, then back off one step; the setting just below the point where the web goes flat is usually the stable one.
Record what you settled on together with the film batch. Film from a different batch can need a different figure, and having the record turns a mystery into a comparison.
Signals that the setting is wrong
Too much tension shows up as edge curl, a print length that shrinks through the run, or bags that seal short because the web relaxes after printing. Too little shows up as wrinkles at an idler, a web that wanders across the eye mark, or a roll that telescopes on the rewind.
A splice is its own signal. A tension step at the splice that the machine cannot absorb will show as a register jump within a few metres, and the defect lands in the middle of the run where it is easiest to miss at inspection.
Where It Applies, and Where It Does Not
This applies to web-fed printing, coating and lamination on flexible film, and to the unwind and rewind of a form-fill-seal machine when the film is printed roll stock. The same reasoning holds for metallised and foil-containing structures, with the caveat that foil has almost no elastic range and will crease rather than stretch.
It does not settle tension for paper or board, where moisture and grain direction dominate, or for stretch film used in wrapping, where the goal is controlled elongation rather than dimensional stability. Those are different processes with different targets, even though the word tension appears in both.
Conclusion
Write web tension settings as a figure per unit width, convert it to the machine’s force at the actual web width, and set the infeed before the unwind and the rewind. Film type decides the window through modulus, and taper decides if the end of the roll behaves like the beginning. When a setting needs constant correction, look for a roller, a gauge band or a splice before changing the number again. The custom roll stock range lists what can be specified on gauge and winding, and the guide to roll defects such as telescope and gauge bands covers the symptoms that most often get mistaken for a tension fault.
For the friction side of web handling, ASTM D1894 sets out how static and kinetic coefficients of friction are measured on plastic film, which is the figure to ask for when a web tracks badly on one side. How roll stock is specified for a printing line is covered in the rollstock film guide.
Frequently Asked Questions
Can I copy web tension settings from one film to another?
No, even when the two films look similar. The setting that matters is the strain it produces, and strain depends on modulus and thickness, both of which change between grades. A polyester film and a polyethylene film of the same thickness sit in very different parts of the window. Use the supplier’s figure for each film and re-check the print length after the change.
Why does the register move when the roll gets small?
Because the brake holds torque while the diameter falls, so the tension rises through the roll unless a taper reduces it. The web stretches progressively and the printed length grows with it. A dancer or load cell that holds force constant will do exactly this. If the drift starts at a similar point on every roll, suspect the taper curve rather than the film or the plates, and check that the diameter input the controller uses matches the roll actually loaded.
Should the rewind run as tight as possible?
No. Rewind only needs to build a roll that stays stable in storage and unwinds cleanly at the customer. Running it tighter than that adds strain after the last print station, which shows up as print length variation between the outside and the core of the roll. Set it to the minimum that produces a firm, non-telescoping roll, and re-check it when the film batch changes.
What does a wrinkle at an idler tell me?
Usually that the web is not flat where it meets that roller, which can come from too little tension, a misaligned idler, or a film with uneven gauge. Check the roller first, then the tension, then the film batch. Wrinkles that appear only on one side of the web often trace back to a roller that is out of parallel rather than to a tension setting.